دانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Synthesis of quantum carbon dots (CQDs) from hard walnut skin by hydrothermal methodسنتز نقاط کوانتومی کربن (CQDs) از پوست سخت گردو با روش هیدروترمال493504504110.22060/ceej.2023.21041.7614FAافسانهشهبازیپژوهشکده علوم محیطی، دانشگاه شهید بهشتی، تهران، ایرانالهامدالپژوهشکده علوم محیطی، دانشگاه شهید بهشتی، تهران، ایرانJournal Article20220209In this study, biocompatible carbon quantum dots (CQDs) were prepared in a single step by hydrothermal method from walnut skin as a carbon source. Particle size, surface chemistry and crystal structure of carbon quantum dots were investigated using FTIR, DLS and XRD analyses and the optical properties of the material were investigated using absorption and fluorescence analyses. The results showed that the quantum dots of synthesized carbon had a good particle size distribution and the average particle size was 5.7 ± 2.5. Also, the effect of temperature on initial carbonization was investigated, which with increasing the temperature of the pyrolysis furnace, the percentage of carbon also increased, which was 46% by weight at 150 °C and 83% by weight at 450 ° C. Due to the fact that, the difference in weight of carbon produced between temperatures of 350 and 450 degrees is very small, and considering the increase of 100 degrees, the temperature of 350 degrees was considered as a suitable temperature for the initial carbonization of walnut shell. The results of the absorption spectrum and fluorescence show that at the 238 wavelength an absorption peak of the sample is observed and the sample shows good fluorescence scattering at the wavelength of 402 nm. According to the results of the studied FT-IR spectrum, the quantum surface of carbon dots is covered by hydrophilic functional groups such as hydroxyl, carbonyl and amine groups, and based on this, the synthesized nanoparticles are expected to show high dispersion in water.در این پژوهش نقاط کوانتومی کربنی (CQDs) زیست سازگار به صورت تک مرحله ای به روش هیدروترمال از پوست گردو به عنوان منبع کربنی تهیه شده است. اندازه ذرات، شیمی سطح و ساختار کریستالی نقاط کوانتومی کربنی با استفاده از آنالیزهای FTIR, DLS و XRD و ویژگی های نوری ماده با استفاده از آنالیزهای جذبی و فلورسانسی بررسی شد. نتایج به دست آمده نشان داد که نقاط کوانتومی کربن سنتز شده از توزیع اندازه ذرات مناسبی برخوردار بوده و میانگین اندازه ذرات 5/7±2/5 بوده است. البته بیشترین توزیع اندازه ذرات مربوط به 5 تا 6 نانومتر است. همچنین اثر دما بر کربونیزاسیون اولیه بررسی شد که با افزایش دمای کوره پیرولیز درصد کربن نیز افزایش پیدا می کند که درصد کربن در دمای 150 درجه 46 درصد وزنی و در دمای 450 درجه 83 درصد وزنی بوده است. البته تفاوت وزنی کربن تولیدی بین دماهای 350 و 450 درجه بسیار اندک است و با در نظر گرفتن افزایش 100 درجهای دما، دمای 350 درجه به عنوان دمای مناسب برای کربونیزاسیون اولیه پوسته گردو در نظر گرفته شد. نتایج اسپکتروم جذبی و فلورسانسی نشان داده که در طول موج 238 یک پیک جذبی از نمونه مشاهده می شود و نمونه نشر فلورسانی مطلوبی در طول موج 402 نانومتر از خود نشان می دهد. با توجه به نتیجه ی طیف FT-IRبررسی شده سطح کوانتوم دات های کربنی از گروه های عاملی آبدوستی همچون گروه های هیدروکسیل، کربونیل و آمین پوشیده شده است و بر همین اساس انتظار می رود نانو ذرات سنتز شده پراکندگی بالایی در آب نشان دهند.https://ceej.aut.ac.ir/article_5041_02c6776504e922729daa6cff6daa8f84.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Seismic performance evaluation of free-standing intake tower using incremental dynamic analysisارزیابی عملکرد لرزهای برجهای آبگیر آزاد-ایستا با استفاده از تحلیل دینامیکی افزایشی505530505210.22060/ceej.2023.19371.7178FAآرماناحمدیدانشکده مهندسی عمران و محیط زیست، دانشگاه تربیت مدرس، تهران، ایرانمحمدعالم باقریدانشکده مهندسی عمران و محیط زیست، دانشگاه تربیت مدرس، تهران، ایرانJournal Article20210104Intake towers form the entrance to the reservoir spillway or diversion system and thus play a key role in the seismic resistance of the whole system. Safety and proper functioning of the intake towers in the event of a major earthquake are very important since the release controlled by the reservoir can help to prevent the failure of the dam after an earthquake by reducing the water pressure. In addition, the current seismic assessment based on the linear elastic constitutive model cannot adequately describe the seismic capacity of intake towers. Thus, to investigate the proper functioning of intake towers in the event of an earthquake, it is necessary to introduce IDA that takes into fully assesses the seismic performance of intake towers based on nonlinear dynamic analysis. In this paper by modeling the intake tower of the Briones dam, intake tower in three conditions of the intake tower, the intake tower-reservoir (outside water) and the tower-reservoir-inside water, under the influence of 12 earthquake records, each of which has a magnitude of seven in the earthquake intensity scale, has been investigated. The displacement at the top of the intake tower, damage to the intake tower body and the maximum tensile stress of the rebar in the intake tower were studied in all three conditions are considered as damage measure (DM), and the results were reported in the form of IDA curves. Then based on the results, the function and different limit-states (key points) of the intake tower structure are determined.<span lang="FA" style="font-family: 'B Nazanin'; font-weight: normal;">برجهای آبگیر ورودی سرریز مخزن یا سیستم انحراف را تشکیل میدهند و در نتیجه نقش کلیدی در مقاومت لرزهای سیستم کلی را بازی میکنند. ایمنی و عملکرد مناسب برجهای آبگیر در صورت وقوع یک زلزله بزرگ بسیار مهم است، زیرا رهایی کنترل شده آب مخزن میتواند از شکست سد پس از زمینلرزه با کاهش فشار آب جلوگیری کند. علاوه بر این ارزیابی عملکرد بر اساس مدل الاستیک خطی، نمیتواند با دقت ظرفیت لرزهای برجهای آبگیر را توصیف کند. از این رو برای بررسی عملکرد مناسب برجهای آبگیر در صورت وقوع یک زلزله ضروری است که </span><span dir="LTR" style="font-size: 9.0pt; line-height: 107%; font-weight: normal;">IDA</span><span style="font-size: 9.0pt; line-height: 107%; font-family: 'B Nazanin'; font-weight: normal;"> </span><span lang="FA" style="font-family: 'B Nazanin'; font-weight: normal;">ارائه شود تا به طور کامل عملکرد لرزهای برجهای آبگیر بر اساس تجزیه و تحلیل دینامیکی غیرخطی تعیین شود. در این مقاله با مدلسازی برج آبگیر سد بریونز، برج آبگیر در سه حالت برج آبگیر تنها، برج آبگیر-مخزن (آب بیرونی) و برج آبگیر-مخزن-آب داخل، تحت اثر 12 رکورد زلزله که هر یک به هفت سطح از شدت زلزله مقیاس گشت، بررسی شده است. جابهجایی بالای برج آبگیر، خرابی بدنه برج آبگیر و ماکزیمم تنش کششی میلگردهای درون برج آبگیر در هر سه حالت به عنوان پارامتر آسیب (</span><span dir="LTR" style="font-size: 9.0pt; line-height: 107%; font-weight: normal;">DM</span><span lang="FA" style="font-family: 'B Nazanin'; font-weight: normal;">) مورد بررسی قرار گرفت و نتایج در قالب منحنیهای </span><span dir="LTR" style="font-size: 9.0pt; line-height: 107%; font-weight: normal;">IDA</span><span style="font-size: 9.0pt; line-height: 107%; font-family: 'B Nazanin'; font-weight: normal;"> </span><span lang="FA" style="font-family: 'B Nazanin'; font-weight: normal;">گزارش شد. سپس بر اساس نتایج، حالات حدی سطوح مختلف (نقاط کلیدی) عملکرد سازه برج آبگیر مشخص شد.</span>https://ceej.aut.ac.ir/article_5052_b751a4ec936acb9c1a1d831ab96d1a78.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Performance of alkali-activated slag and pumice mortars against chloride ions penetration in the Persian Gulfبررسی عملکرد ملاتهای سرباره و پومیس قلیافعال در برابر نفوذ یونهای کلراید در محیط خلیجفارس531554505510.22060/ceej.2023.20867.7552FAمحسنجعفری ندوشندانشکده مهندسی عمران و منابع زمین، دانشگاه آزاد اسلامی، واحد تهران مرکزی، تهران، ایرانعلی اکبررمضانیان پوردانشکده مهندسی عمران و محیط زیست، دانشگاه صنعتی امیرکبیر، تهران، ایرانJournal Article20211209<span style="letter-spacing: .05pt;">Considering the successful usage of alkali-activated mortars in several countries and limited research on the durability of these materials, in this paper, the permeability and durability of alkali-activated slag and pumice mortar in chloride environments have been studied. To investigate the mechanical properties and permeability of alkali-activated slag and pumice mortars tests such as workability, compressive strength, capillary water absorption, water absorption, chloride ion penetration in the Persian Gulf environment and mercury intrusion porosimetry have been conducted. The results show that the compressive strength of alkali-activated slag mortar containing potassium hydroxide was slightly higher than the compressive strength of samples containing sodium hydroxide. In addition, the use of 10% pumice instead of slag has increased the compressive strength of alkali-activated slag mortar. Also, the 91-day compressive strength of alkali-activated mortars cured in the water was 48.4% higher than those cured in the air. In general, the diffusion coefficient of chloride ions in alkali-activated slag mortars was lower than the diffusion coefficient of chloride ions in Portland cement mortar, which was due to less porosity in alkali-activated slag mortars and the denser structure. Also, alkali-activated mortars containing 90% of slag and 10% of pumice had the lowest diffusion coefficient of chloride ions and Portland cement mortar showed the highest one, which was well matched with the result of capillary water absorption coefficient.</span>با توجه به سابقه موفق به کارگیری ملات های قلیافعال در برخی کشورها در سال های اخیر و تحقیقات محدود صورت گرفته بر روی دوام این مصالح، در این مقاله به بررسی خصوصیات نفوذپذیری و دوام در برابر نفوذ یونهای کلراید پرداخته شده است. به منظور بررسی خواص مکانیکی و نفوذپذیری ملات های قلیافعال حاوی سرباره کوره آهنگدازی و پوزولان طبیعی پومیس در مطالعات آزمایشگاهی از آزمایشهایی مانند کارایی، مقاومت فشاری، جذب آب موئینه، جذب آب حجمی، نفوذ یونهای کلراید در محیط واقعی خلیج فارس و تخلخل سنجی به روش تزریق جیوه بهره گرفته شده است. نتایج به دست آمده نشان می دهد که مقاومت فشاری آزمونه های ملات قلیافعال حاوی هیدروکسیدپتاسیم در مقایسه با مقاومت فشاری آزمونه های حاوی هیدروکسیدسدیم کمی بیشتر بوده است. ضمناً استفاده از 10 درصد پومیس به جای سرباره باعث افزایش مقاومت فشاری ملات قلیافعال شده است. همچنین مقاومت فشاری 91 روزه آزمونه های ملات سرباره قلیافعال عمل آوری شده در آب، 48/4 درصد بیشتر از آزمونه های عمل آوری شده در هوا بوده است. به طور کلی ضریب انتشار یونهای کلراید در ملات های قلیافعال کمتر از ضریب انتشار یونهای کلراید در ملات سیمان پرتلندی شاهد بوده که این موضوع به دلیل وجود حفرات کمتر در ملاتهای قلیافعال و ساختار متراکمتر ملات های قلیافعال در مقایسه با ملات سیمان پرتلندی شاهد بوده است. همچنین ملات قلیافعال حاوی 90 درصد سرباره و 10 درصد پومیس کمترین و ملات سیمان پرتلندی بیشترین ضریب انتشار یونهای کلراید را از خود نشان داده اند که نتایج ضریب جذب آب مویینگی نیز موید این موضوع بوده است.https://ceej.aut.ac.ir/article_5055_1d689977f75a568a6198c28bba05005f.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Splitting Test on Masonry Cores and modeling of the Confined mortar behavior based on fracture energyآزمایش شکافت استوانه بنایی و مدلسازی رفتار محصور شده ملات بر مبنای انرژی شکست555582505710.22060/ceej.2023.21192.7647FAحمیدتوانایی فردانشکده فنی، دانشگاه رازی، کرمانشاه، ایرانامیرهوشنگاخویسیدانشکده فنی، دانشگاه رازی، کرمانشاه، ایرانJournal Article20220306The in situ evaluation of the masonry's mechanical properties is a very complicated task. A viable alternative is based on the use of brick cores including a central mortar layer lying on a symmetry plane. In fact, these specimens can be extracted very easily by cutting cores spanning two bricks at least. The obtained core is then subjected to a splitting test with a setup providing a different inclination of the mortar layer with respect to the loading plane. This type of test is similar to a diagonal wallet test and induces a mixed compression–shear stress state in the central mortar layer. Here, This test is used for masonry with sand and cement mortar. By using a Mohr-Coulomb failure criterion the test result can be interpreted in order to obtain all the mechanical properties of the masonry. This test can be a good alternative to other semi-destructive tests, especially the shove test. The latter test has a defect, that’s due to the lack of effect of dilatancy in the shear behavior of mortar in the shove test, the values obtained in terms of cohesion and friction angle will be greater than the actual value. In the following, a 3D continuous micromodel is presented in order to predict unreinforced masonry behavior. Due to the difference in the modulus of elasticity, the Poisson ratio and the thickness of the brick and mortar, several efforts have been made to simulate the compressive behavior of the masonry using different models with different goals and results. To examine this behavior, which is influenced by the interaction of units and mortar, in one hand, two-dimensional models are not able to consider the 3D confined effect. On the other hand, the three-dimensional models are not able easily to control the effect of 3D confined and dilatation explicitly. The proposed model is based on the concept of micro-plane and is developed to model failure in masonry structures.در این مقاله از تست برزیلی (شکافت) که یک آزمایش نیمه مخرب بوده و حداقل دست خوردگی را در سازه ایجاد می کند، جهت تخمین پارامترهای مقاومتی بنایی های با ملات ماسه و سیمان استفاده می گردد. در این شیوه، به وسیله استخراج مغزه های دارای یک بندِ ملات، و اجرای تست برزیلی تحت زوایای مختلف ملات نسبت به راستای اصلی، می توان پارامترهای مقاومتی بنایی را (c و ) استخراج کرد. این تست را می توان جایگزین مناسبی برای سایر تست های نیمه مخرب خصوصاً تست برش ملات به شمار آورد. تست اخیر نواقصی دارد که عمده آن وجود عدم لحاظ اثر اتساع در ملات است. نقص مذکور، موجب تشدید تنش عمودی موجود بر روی آجر مورد آزمایش شده و در نتیجه مقادیر پارامترهای مقاومتی را بیشتر از مقدار واقعی، برآورد می کند. در ادامه یک ریزمدل پیوسته سه بعدی جهت پیش بینی رفتار بنایی غیرمسلح در فشار، ارائه می گردد. با توجه به تفاوت در مدول الاستیسیته، ضریب پواسون و ضخامت دو مصالح آجر و ملات در بنایی، تلاش های متعددی برای شبیهسازی رفتار فشاری بنایی انجام شده است. برای بررسی این رفتار که تحت تأثیر اندرکنش واحدها و ملات است، مدل های دو بعدی قادر به لحاظ محصورشدگی سه محوره ملات نیستند. از طرفی مدل های سه بعدی موجود به سادگی قادر به کنترل اثر اتساع به صورت صریح و لحاظ محصورشدگی سه محوره نمی باشند. مدل ارائه شده بر مبنای مفهوم ریز صفحه (چند صفحه) است و برای مدلسازی شکست در سازه بنایی در اثر فشار توسعه می یابد. در ادامه توانایی مدل ارائه شده در مقابل نتایج آزمایشگاهی و سایر مدل های عددی، بررسی شده و جهت مدلسازی کار آزمایشگاهی حاضر استفاده میگردد. مقایسه نتایج، دقت مناسب نتایج حاصل از مدل عددی پیشنهادی و قابلیت اجرای تست مغزه در بناییهای آجری با ملات ماسه-سیمان را نشان میدهد.https://ceej.aut.ac.ir/article_5057_d52e30b07dac358497719fb635e23f9f.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Investigation on properties of cold recycled asphalt mixtures reinforced with polypropylene fibersارزیابی خصوصیات مخلوطهای آسفالتی بازیافتی سرد تسلیح شده با الیاف پلی پروپیلن583602505810.22060/ceej.2023.20436.7441FAمحمدرضاصبوریدانشکده مهندسی عمران، دانشگاه صنعتی شریف، تهران، ایرانمحمدصادقیدانشکده مهندسی عمران، دانشگاه صنعتی شریف، تهران، ایرانJournal Article20210902<span style="letter-spacing: .05pt;">Despite substantial environmental and economic benefits, cold recycling of asphalt pavements is not common due to some poor field performance reports. This study investigates the effect of fiber reinforcement on the performance of cold recycled mixtures. For this purpose, cold recycled mixtures were reinforced using polypropylene fibers at two different lengths and three different contents. Indirect tensile strength, IDEAL-CT, and semicircular bending tests were carried out to find the optimum length and content of the fiber. The effect of cement on the performance of fiber-reinforced mixtures was also evaluated. The results show that although the use of polypropylene fibers reduces the wet strength by up to 54%, it can increase the dry strength by up to 39%. The results also indicate a significant improvement in fracture indices obtained from IDEAL-CT and SCB tests in the presence of fiber. The crack tolerance index was 3.5 times and the flexibility index was 2.8 times higher at the optimum fiber content and length compared with the control mixture. It was also concluded that the addition of cement to fiber-reinforced mixture can eliminate the adverse effect of fiber on moisture sensitivity while maintaining fracture properties similar to the control mixture. The study results show that the combined use of fibers and cement can lead to an economical cold recycled mixture with reduced emulsified asphalt content and improved mechanical properties.</span>برخلاف مزایای قابل توجه بازیافت سرد روسازیهای آسفالتی، به دلیل ضعفهای عملکردی، استفاده از آن چندان متداول نیست. در این پژوهش، اثر الیاف پلی پروپیلن و همچنین اثر همزمان الیاف پلی پروپیلن و سیمان در بهبود خصوصیات عملکردی مخلوطهای بازیافتی سرد امولسیونی تحقیق شده است. بدین منظور، مخلوطهای بازیافتی سرد با استفاده از الیاف پلی پروپیلن در دو طول و سه مقدار مختلف تسلیح شده و آزمایشهای مقاومت کششی غیرمستقیم، شاخص تحمل ترک و خمش تیرچهی نیمدایرهای برای یافتن طول و مقدار بهینهی الیاف و نیز بررسی عملکرد مخلوطهای الیافی انجام شد. همچنین اثر همزمان الیاف (در درصد و طول بهینه) و سیمان بررسی شد. نتایج نشانگر آن است که اگرچه استفاده از الیاف پلی پروپیلن، مقاومت تر را در بدترین حالت تا 54 درصد کاهش میدهد، در بهترین حالت مقاومت خشک را تا 39 درصد افزایش میدهد. نتایج همچنین نشانگر امکان افزایش قابل ملاحظهی شاخصهای شکست در آزمایشهای IDEAL-CT و SCB با استفاده از الیاف پلی پروپیلن است. مقادیر شاخصهای تحمل ترک و شاخص انعطافپذیری برای مخلوطهای دارای الیاف بهینه به ترتیب 3/5 و2/8 برابر بزرگتر از مقادیر مخلوط کنترل پایه بود. همچنین مشاهده شد که استفادهی همزمان از الیاف و سیمان توانایی حفظ و ارتقای اثرات مثبت سیمان و جبران کاهش شاخصهای شکست ناشی از افزودن سیمان را دارد و در عین حال حساسیت رطوبتی متاثر از الیاف را برطرف میکند. نتایج نشانگر این است که استفادهی همزمان از الیاف و سیمان میتواند به رویکردی اقتصادی جهت کاهش مقدار امولسیون بهینه و در عین حال ارتقای خصوصیات عملکردی مخلوط بازیافتی سرد منجر شود.https://ceej.aut.ac.ir/article_5058_a8eac0ce94ed0d61c798c2f113952521.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Evaluating the FIDIC's termination for convenience clause in General Conditions under common law in Iranian civil law system for Construction Contractsارزیابی ماده فسخ به مصلحت در شرایط عمومی پیمان پروژههای ساخت فیدیک، بر اساس قوانین عرفی در سیستم قانون مدنی ایران603618505910.22060/ceej.2023.19087.7063FAنویدباقریان مرندیدانشکده مهندسی، واحد علوم و تحقیقات، دانشگاه آزاد اسلامی، تهران، ایرانمهدیروانشادنیادانشکده مهندسی، واحد علوم و تحقیقات، دانشگاه آزاد اسلامی، تهران، ایرانمحمد رضااکبرزاده توتونچیدانشکده فنی و مهندسی، دانشگاه فردوسی، مشهد، ایرانJournal Article20201004<span style="letter-spacing: .05pt;">The Iran civil code is based mainly on the Egyptian Civil Law (ECL), which is itself derived from two principal sources like French civil law and Islamic law. On the other hand, the general conditions of contracts published by the Fédération Internationale des Ingénieurs-Conseils or International Federation of Consulting Engineers (FIDIC), which are based on common law principles and this standard form of contract, have been applied in large construction projects in Iran. Due to Iran's legal system is rooted in civil law, FIDIC forms of contract may face serious challenges. This research, through a comparative method, has analyzed the Egypt Civil Code (ECC) and Iran (as two members of the Islamic legal system) for better decisions in FIDIC-based contracts. Our study offers some strategies for modification of the FIDIC 1999 Red Book [FIDIC (CONS)] and also the Iran Civil Code for construction contracts, which are associated with the termination for convenience clause. Therefore, with a better understanding of the termination for convenience by the employer clause, which has been referred to in many contractual claims in arbitration centers and courts, can be prevented disputes. Moreover, this study is useful for other Middle East countries because most of them follow civil law jurisdictions.</span><span lang="FA" style="font-family: 'B Nazanin'; font-weight: normal;">قانون مدنی ایران برداشتی از قانون مدنی مصر است که این قانون نیز خود از قانون مدنی فرانسه و فقه اسلام استخراج شده است، سالها است که در تنظیم قراردادهای پروژههای بزرگ ساخت در کشور ایران از شرایط عمومی پیمان استاندارد منتشر شده توسط فدراسیون بینالمللی مهندسان مشاور (فیدیک) که بر مبنای حقوق عرفی یا سابقه قضائی (کامن لا) استوار است، استفاده میشود. این در حالی است که این نوع قراردادها در سیستمی که مبنای تصمیمگیری مراجع قضائی در آن قانون مدنی ایران است، با چالشهای جدی مواجه هستند. بنابراین ضروری است ذی نفعان فعال در پروژههای ساخت ایران با تداخلات رویکرد فیدیک در مقابل قانون زمینه مدنی اطلاع کافی داشته باشند. در این مقاله با مقایسه تطبیقی آیین مدنی مصر و ایران (به عنوان دو کشور با سیستم قانونی برگرفته از اسلام) با شرایط عمومی پیمان فیدیک به تداخلات رویکرد رسیدگی قضائی در دو نظام حقوقی مختلف پرداخته شده است. نتیجه این مطالعات ارائه چند پیشنهاد در قانون مدنی ایران و کتاب قرمز فیدیک 1999 (فیدیک ساخت) در خصوص ماده فسخ قرارداد به مصلحت، گردیده است. از آنجایی که در اختلافات قراردادهای ساخت بیشتر به ماده فسخ قرارداد در دادگاهها و مراجع داوری استناد شده است، میتوان این انتظار را داشت که پیمانکاران با درک بهتر ماده فسخ به مصلحت کارفرما در قراردادهای خود از بروز اختلافات در این زمینه پیشگیری کنند، به علاوه، این مطالعه برای سایر کشورهای خاورمیانه مفید است زیرا بیشتر آنها از قلمروهای قانون مدنی پیروی میکنند.</span>https://ceej.aut.ac.ir/article_5059_c29ae9c64e5d5989214e84a2f8db5a65.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Investigating the dynamic response of deep mixing columns and gravel columns in liquefiable layer with different thicknessبررسی پاسخ دینامیکی ستونهای اختلاط عمیق و ستونهای شنی در لایه روانگرا با ضخامت مختلف619640507010.22060/ceej.2023.21772.7821FAقلیاسدزاده خوشه مهردانشکده فنی و مهندسی، دانشگاه ارومیه، ارومیه، ایرانهادیبهادریدانشکده فنی و مهندسی، دانشگاه ارومیه، ارومیه، ایرانJournal Article20220914<span style="letter-spacing: .05pt;">Liquefaction is one of the most devastating Geotechnical phenomena that severely damage vital structures and lifelines. An accurate understanding of the dynamic response of the site prone to liquefaction and improved with different modern methods and comparing it with the unimproved site improves the ability of engineers to choose the appropriate improvement method. Before construction, it is necessary to solve the geotechnical problem. Among the methods of land improvement to deal with liquefaction, gravel columns and deep mixing columns can be mentioned. In this study, the results of 1g shaking table tests by a flexible box on the foundation located on the liquefiable ground surface and reinforced with the aforementioned techniques have been investigated. The dynamic responses of the reinforced ground in different thicknesses of the liquefiable layer and the different frequencies of the input movement have been investigated based on stress-strain behavior, secant shear modulus of the soil and excess pore water pressure versus shear strain. The results of the tests show that the thickness of the liquefiable layer has a considerable effect on the dynamic responses of the soil, including the shear behavior and the shear modulus of the soil. By increasing the thickness of the liquefiable layer, the values of the secant shear modulus and shear strain of the improved mass decrease and increase respectively. Also, the dynamic performance of deep mixing columns in thicker layers is more suitable compared to gravel columns, and at lower thicknesses, the dynamic behavior of gravel columns approaches that of deep mixing columns. </span>روانگرایی یکی از مخربترین پدیدههای ژئوتکنیکی میباشد که باعث ایجاد خسارت سنگین به سازهها و شریآنهای حیاتی میشود. شناخت درست از پاسخ دینامیکی ساختگاه بهسازی شده با روشهای نوین و مقایسه آن با حالت بهسازی نشده میتواند توانایی مهندسان برای انتخاب روش بهسازی مناسب و مختص هر ساختگاه را ارتقا دهد. قبل از احداث سازهها بر روی زمین مستعد روانگرایی، ضرورت بهسازی ساختگاه و برطرف کردن مشکل ژئوتکنیکی دارای اهمیت میباشد. از جمله روشهای نوین بهسازی میتوان به استفاده از ستونهای اختلاط عمیق و ستونهای شنی اشاره کرد. در این مطالعه نتایج یک سری آزمایشهای میزلرزه در محیط g 1 توسط جعبه انعطافپذیر بر روی فونداسیون مستقر در سطح زمین قابل روانگرا و مسلح شده با دو نوع تکنیک ستونهای اختلاط عمیق و ستونهای شنی مورد بررسی قرار گرفته است. پاسخهای دینامیکی سیستم زمین مسلح شده و فونداسیون در ضخامتهای مختلف لایه روانگرا و به علاوه فرکانس حرکت ورودی متفاوت در قالب رفتار تنش-کرنش، تغییرات مدول برشی سکانتی، اضافه فشار آب حفرهای و کرنش برشی مورد ارزیابی قرار گرفته است. نتایج آزمایشها نشان میدهد که ضخامت لایه روانگرا بر پاسخهای دینامیکی خاک از جمله رفتار تنش-کرنش خاک و پارامتر مدول برشی سکانتی تاثیر قابل تأملی میگذارد. با افزایش ضخامت لایه روانگرا مقادیر مدول برشی و کرنش برشی توده بهسازی شده به ترتیب کاهش و افزایش پیدا میکند. همچنین عملکرد دینامیکی ستونهای اختلاط عمیق در لایههای ضخیم در مقایسه با ستونهای شنی مناسبتر میباشد، در عین حال در ضخامتهای کمتر رفتار دینامیکی ستونهای شنی به ستونهای اختلاط عمیق نزدیکتر میشود.https://ceej.aut.ac.ir/article_5070_d6ca879cbecc57b53c2047a063ffdd27.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Effect of Zeolite on the Compressive Strength and Durability Properties of Roller-Compacted Mass Concreteاثر زئولیت بر مقاومت فشاری و خصوصیات دوام بتن غلتکی حجیم641664507810.22060/ceej.2023.21999.7875FAعلیصرافیدانشکده مهندسی عمران، دانشگاه تهران، تهران، ایرانسید مهدیزهراییدانشکده مهندسی عمران، دانشگاه تهران، تهران، ایران0000-0003-2759-2424امیرمحمدرمضانیان پوردانشکده مهندسی عمران، دانشگاه تهران، تهران، ایرانJournal Article20221208<span style="letter-spacing: .05pt;">Roller Compacted Mass Concrete is one of the special types of concrete that has a low amount of cement in its mixture proportion in order to reduce the heat caused by the hydration reaction. This increases the permeability of roller-compacted concrete compared to conventional concrete. The increase in permeability also leads to the entry of destructive ions into the concrete of mass structures and ultimately the instability of these structures. Supplementary cementitious materials such as zeolite can reduce permeability, so in this research, the effect of replacing a part of cement with zeolite on the durability and mechanical properties of roller-compacted concrete has been investigated. First, chemical analysis and the pozzolanic activity of zeolite were investigated. Then, in order to evaluate the effect of zeolite on the properties of concrete, roller-compacted concrete specimens were made in four mixture proportions with replacement percentages of 0%, 15%, 30% and 40% of cement with zeolite and subjected to compressive strength, water penetration depth, water absorption, Rapid Chloride Permeability Test (RCPT), electrical resistivity, Ultrasonic Pulse Velocity (UPV). The workability of the roller-compacted concrete mixtures was also determined by the V.B. time test. The results showed that according to RCPT, water penetration depth and electrical resistivity tests, replacing 15% of cement weight with zeolite reduces permeability and significantly improves the durability properties of roller-compacted concrete. Also, increasing the percentage of zeolite reduces the compressive strength of the specimens.</span>بتن غلتکی کم سیمان یکی از انواع بتنهای خاص است که به جهت کاهش حدود 2 برابری حرارت ناشی از واکنش هیدراته شدن، مقدار سیمان در نسبت مخلوط آن کم است. این موضوع باعث افزایش قابل توجه نفوذپذیری بتن غلتکی نسبت به بتن معمولی میشود. افزایش نفوذپذیری نیز ورود یونهای مخرب (نظیر یونهای کلراید، سدیم، پتاسیم و کلسیم) به بدنه بتنی سازههای حجیم را موجب میشود و در نهایت عدم پایداری این سازهها را به دنبال دارد. پوزولانها مانند زئولیت میتوانند نفوذپذیری را کاهش دهند، از این رو در تحقیق حاضر، تأثیر جایگزینی بخشی از سیمان با زئولیت بر مقاومت فشاری و خصوصیات دوام نظیر نفوذ تسریع شده یون کلراید، عمق نفوذ آب، جذب آب، مقاومت الکتریکی و سرعت پالس اولتراسونیک بتن غلتکی بررسی شده است. ابتدا آنالیز شیمیایی و واکنش پوزولانی زئولیت بررسی شدند. سپس به منظور ارزیابی تأثیر زئولیت بر خواص بتن، نمونههای بتن غلتکی در چهار نسبت مخلوط با درصدهای جایگزینی %0، %15، %30 و 40% سیمان با زئولیت ساخته شدند و تحت آزمایشهای مقاومت فشاری، عمق نفوذ آب، جذب آب، نفوذ تسریع شده یون کلراید (RCPT)، مقاومت الکتریکی، سرعت پالس اولتراسونیک (UPV) قرار گرفتند. کارایی مخلوطهای بتن غلتکی نیز از طریق آزمایش میز وی بی تعیین شد. نتایج نشان دادند که بر طبق آزمایشهای RCPT، عمق نفوذ آب و مقاومت الکتریکی، جایگزینی 15% وزن سیمان با زئولیت باعث کاهش نفوذپذیری و بهبود چشمگیر خصوصیات دوامی میشود. همچنین افزایش درصد زئولیت، مقاومت فشاری نمونهها را کاهش میدهد. مقایسه با تعداد 96 نمونه مکعبی 15 سانتیمتری صورت گرفته است. بر اساس نتایج مقاومت فشاری 7 روزه، جایگزینی سیمان با 15%، 30% و 40% زئولیت به ترتیب باعث کاهش 45/7%، 56% و 61/7% مقاومت فشاری نسبت به نمونه شاهد شده است. این مقادیر کاهش برای مقاومت فشاری 28 روزه به ترتیب 24/7%، 39/5% و 51/6%، برای نتایج 56 روزه به ترتیب 27%، 3/34% و 46/1% و برای نتایج 91 روزه نیز، به ترتیب 21/2%، 35/3% و 45/3% میباشد.https://ceej.aut.ac.ir/article_5078_cbc895f6d9aeecfe008ce368bbd37902.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Damage detection in structures using finite element model updating based on changes in wavelet transform coefficients of a correlation functionشناسایی آسیب در سازهها با استفاده از بروزرسانی مدل المان محدود با استفاده از تغییرات ضرایب تبدیل موجک تابع همبستگی665680507510.22060/ceej.2023.20796.7528FAمحسنصادقیاندانشکده مهندسی دریا، صنعتی امیرکبیر، تهران، ایراناکبراسفندیاریدانشکده مهندسی دریا، صنعتی امیرکبیر، تهران، ایرانمنوچهرفدویدانشکده مهندسی دریا، صنعتی امیرکبیر، تهران، ایرانJournal Article20211118In this paper, an innovative finite element updating method is presented based on the sensitivity of wavelet transform coefficients of correlations function structural parameters is proposed to identify the damage. The Quasi-linear sensitivity of the wavelet coefficients of the WTCF concerning the structural parameters is evaluated based on incomplete measured structural responses. This WTCF sensitivity is more sensitive to local structural changes than the wavelet transform function response sensitivity. The model is updated by the wavelet transform coefficients achieved in the frequency range in the vicinity of the resonances, in which damping and incomplete measurements have no significant effect on the results of the parameter estimation. The proposed algorithm is used to estimate the structural parameters of the frame model. By the solution of the sensitivity equation through the Least-squares method, the finite element model of the structure is updated for estimation of the location and severity of structural damages, simultaneously. The proposed method was successfully applied to a 2D frame model using simulated data contaminated by measurement and modeling errors. The robustness of the method against modeling and mass measurement errors is investigated by adding random errors to the mass parameters of the frame model.در این مقاله، روشی نوآورانه جهت بروزرسانی مدل المان محدود مبتنی بر حساسیت ضرایب تبدیل موجک تابع همبستگی نسبت به پارامترهای سازه<strong></strong>ای، جهت شناسایی آسیب ارائه شده است. حساسیت شبه خطی ضرایب موجک تابع همبستگی بر اساس پارامترهای سازه ای، با توجه به پاسخهای سازه ای اندازهگیری شده ناقص، ارزیابی شده است. معادله حساسیت پیشنهادی بر اساس تبدیل موجک تابع همبستگی در مقایسه با تابع تبدیل موجک پاسخ سازه، نسبت به تغییرات محلی سازه، حساسیت بیشتری دارد. ضرایب تبدیل موجک به دست آمده در محدوده فرکانس های طبیعی و همچنین در مجاورت رزونانس ها که در آن میرایی و اندازهگیریهای ناقص تأثیر قابلتوجهی بر نتایج تخمین پارامتر ندارند، جهت شناسایی آسیب در سازه مورد نظر بروزرسانی شده است. الگوریتم پیشنهادی، برای تخمین پارامترهای سازهای مدل قاب استفاده شده است. با حل معادله حساسیت به روش حداقل مربعات، مدل اجزای محدود سازه برای تخمین مکان و شدت آسیب های سازه به طور همزمان بروزرسانی شده است. توانایی روش به صورت عددی، بر روی سازه قاب، در چندین سناریوی آسیب مورد مطالعه قرار گرفته شده است. نتایج، قدرتمندی روش در تشخیص آسیب در برابر خطای مدل سازی و اندازه گیری جرم با افزودن خطاهای تصادفی به شبیه سازی داده های مدل آسیب دیده و پارامتر جرم را نشان می دهد.https://ceej.aut.ac.ir/article_5075_015308d69dec22fdb949b18f7bc7e104.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Experimental study of shear retrofit of RC beam-column joints using external post-tensioned boltsبررسی آزمایشگاهی تقویت برشی اتصالات تیر-ستون کناری بتن آرمه به کمک بولتهای پستنیده خارجی681700507310.22060/ceej.2023.21181.7641FAاحسانتوسلیدانشکده مهندسی عمران، دانشگاه سمنان، سمنان، ایران0000-0002-4508-766Xامیدرضائی فردانشکده مهندسی عمران، دانشگاه سمنان، سمنان، ایران0000-0002-4753-7775علیخیرالدیندانشکده مهندسی عمران، دانشگاه سمنان، سمنان، ایران0000-0001-7802-2013Journal Article20220303RC beam-column joints play a crucial role in transferring gravity and lateral loads from beam to column. By examining damaged buildings in recent earthquakes, RC beam-column joints are among the most vulnerable members of RC moment frames. Joint failure can pose a threat to the structure, ending up destroying the structure. The main type of failure of RC joints is shear failure due to the lack of transverse reinforcement and confinement in this area. The laboratory program of the current study suggests external post-tensioned bolts to retrofit RC joints. External post-tensioned bolts increase the confinement and enlargement of the joint panel zone and subsequently eliminate the deficient shear joints. Regarding the forces applied to the joint panel zone are implemented diagonally, the external post-tensioned bolts were used in two horizontal-vertical (HV) and diagonal (Di) patterns around the joint. The horizontal-vertical pattern was chosen owing to placing the resultants of the retrofit bolts forces in the direction of the applied forces. Furthermore, the diagonal pattern was adopted due to the placement of the retrofit bolts in the direction of the applied forces. The testing program includes four RC beam-column joint specimens with half-scale. One specimen was constructed as a standard criterion with all seismic requirements, and three specimens were made at the joint without implementing transverse reinforcement. One deficient specimen was used as a control specimen, and two specimens were subjected to cyclic loading after retrofitting by the proposed patterns. In order to investigate the effect of the proposed method, parameters such as; the force-displacement hysteresis response, energy absorption and damping value of the specimens were considered. The test results confirm the significant effect of the retrofit system against seismic loading. Accordingly, the failure was exited from the joint panel zone and transferred to the beam in retrofitted specimens. The final capacity of the retrofitted specimens increased by nearly 50% and their energy absorption by about 200%. In addition, the damping values and the ductility factors increased by about 100% and 32% in retrofitted specimens, respectively.اتصالات تیر-ستون بتن آرمه به دلیل نقش کلیدی که در انتقال بارهای ثقلی و جانبی از تیر به ستون دارند از اهمیت بالایی برخوردارند. با بررسی ساختمانهای خسارت دیده در زلزله های اخیر مشخص شده است که اتصالات تیر-ستون بتن آرمه جزء آسیب پذیرترین اعضای قاب های خمشی بتن آرمه میباشند. عمده ترین نوع شکست اتصالات بتن آرمه، شکست برشی ناشی از عدم اجرا و یا ناکافی بودن آرماتورهای عرضی در محل چشمه اتصال می باشند. در این پژوهش که شامل یک برنامه آزمایشگاهی می باشد، سعی شده است روشی کاربردی و موثر جهت مقاوم سازی و بهسازی اتصالات دارای ضعف برشی در محل چشمه اتصال ارائه گردد. بر همین اساس و با توجه به بهبود خواص مکانیکی بتن محصور شده نسبت به بتن محصور نشده، استفاده از سیستم پستنیده خارجی پیشنهاد گردید. در سیستم پستنیده خارجی از دو الگوی افقی-قایم و مورب بولت های پستنیده در اطراف چشمه اتصال استفاده شد. اجرای پستنیده بولت های تقویتی در اطراف اتصال، موجب افزایش محصور شدگی هسته اتصال شد. علاوه بر این، سیستم پستنیده خارجی موجب بزرگتر شدن ابعاد اتصال شد که این موضوع موجب توزیع تنشها در سطح بزرگتری از مقطع شد. برنامه ی آزمایشی شامل چهار نمونه اتصال تیر-ستون بتن آرمه با مقیاس 1/2 بود که دو نمونه به عنوان نمونه های کنترلی و دو نمونهی دیگر به روش های پیشنهادی مورد تقویت قرار گرفتند. به منظور ارزیابی عملکرد لرزهای سیستم تقویت پیشنهادی، پارامترهای لرزه ای نمونه ها شامل: ظرفیت نهایی، میزان جذب انرژی، سختی، میرایی و ضریب شکل پذیری هر یک از نمونه ها استخراج و مورد مقایسه قرار گرفتند. نتایج آزمایشات عملکرد بسیار مناسب سیستم های تقویتی در برابر بارهای لرزه ای را نشان دادند، به گونه ای که در نمونه های تقویتی، خرابی از چشمه اتصال خارج و به داخل تیر منتقل شد. ظرفیت نهایی نمونه های تقویتی در حدود 50% و میزان جذب انرژی آنها نیز در حدود 200% افزایش یافت. همچنین، مقادیر میرایی و ضریب شکل پذیری نمونه های تقویتی به ترتیب در حدود 100% و 32% افزایش پیدا کردند.https://ceej.aut.ac.ir/article_5073_1c88ce6f0a26727d26903fb256437aa3.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Numerical investigation of effective parameters on the behavior of concrete-filled steel tubular gusset plate connectionsبررسی عددی پارامترهای مؤثر بر رفتار اتصال ورق گاست به مقاطع لولهای فولادی پر شده با بتن701722507910.22060/ceej.2023.20837.7545FAمیلادابراهیم نژاد شلمانیدانشکده فنی و مهندسی شرق، دانشگاه گیلان، رودسر، ایرانعلیراضی احمدسراییدانشکده فنی، دانشگاه علم و فرهنگ، رشت، ایرانپویاآرزومند لنگرودیدانشکده فنی، دانشگاه آزاد اسلامی، واحد تهران جنوب، تهران، ایران0000-0002-7345-3743Journal Article20211202Concrete-filled steel tubular (CFST) gusset plate connection is a commonly used method in which the plates are welded directly to the columns. Due to the importance of stress distribution and energy absorption capacity on the behavior of the mentioned connections, in the present study, numerical analysis of the behavior of these connections under different loadings has been investigated. The studied variables include the thickness of the gusset plate, the compressive strength of the concrete, the D/t (diameter to thickness) ratio of CFST, and the type of loading. The results show that although filling hollow tubular sections with concrete prevents the local buckling of the steel wall, the use of concrete with higher compressive strength does not always lead to increased load capacity and energy absorption, so in many of the studied models, the energy absorption capacity decreases by 18% to 30%. On the other hand, the results showed that the diameter-to-thickness ratio has a significant effect on the energy absorption capacity of the simulated connections so by increasing this ratio, the energy absorption capacity has decreased in the range of 76% to 91%. Also, the loading condition is effective in the load-bearing capacity and the energy absorption of the structure. So that in the case of eccentric tension and in-plane bending, the energy absorption capacity is reduced by 53% and 86%, respectively, compared to axial tension loading.اتصال مقاطع لولهای فولادی پر شده با بتن (Concrete Filled Steel Tube) به ورق گاست (Gusset plate)، یک روش اتصال متداول است که در آن، صفحات مستقیماً به وجوه ستون جوش میشوند. نظر به اهمیت چگونگی توزیع تنش و ظرفیت جذب انرژی بر رفتار اتصال مذکور، در مطالعهی حاضر به تحلیل عددی رفتار این اتصال تحت بارگذاریهای مختلف پرداخته شده است. متغیرهای مورد بررسی شامل ضخامت ورق گاست، مقاومت فشاری بتن، نسبت قطر به ضخامت لوله فولادی متصل به ورق گاست و نوع بارگذاری میباشد. نتایج حاصل نشان میدهد اگر چه پر کردن مقاطع لولهای توخالی با بتن کمانش موضعی جدارهی فولادی را به تعویق میاندازد، اما استفاده از بتن با مقاومت فشاری بیشتر همواره منجر به افزایش میزان جذب انرژی نمیشود، به طوری که در بسیاری از مدلهای مورد مطالعه کاهش ظرفیت جذب انرژی 18 تا 30 درصدی اتفاق افتاده است. از سوی دیگر نسبت قطر به ضخامت نقش تاثیرگذاری بر میزان ظرفیت جذب انرژی اتصالات داشته و با افزایش این نسبت، ظرفیت جذب انرژی بین 76 تا 91 درصد کاهش مییابد. همچنین نحوه اعمال بار نیز بر رفتار این اتصالات مؤثر است، به نحوی که در حالت بارگذاری کششی برون محور و خمش صفحهای، ظرفیت جذب انرژی در مقایسه با حالت بارگذاری کشش محوری به ترتیب 53 و 86 درصد کاهش یافته است. لذا میبایست به منظور پیشبینی درست از ظرفیت باربری و میزان جذب انرژی نهایی سازه، توجه لازم به این موضوع در فرآیند طراحی صورت پذیرد.https://ceej.aut.ac.ir/article_5079_4d491f23796cc749aa9c468e563db651.pdfدانشگاه صنعتی امیرکبیرنشریه مهندسی عمران امیرکبیر2588-297X55320230522Effect of alkaline solution to binder ratio on the fracture parameters of lightweight geopolymer concrete based on fly ashتاثیر نسبت فعال کننده به چسب بر پارامترهای شکست بتن ژئوپلیمری سبک بر پایه خاکستر بادی723738508110.22060/ceej.2023.21003.7594FAمحمد رضاعباسی زرگلهدانشکده مهندسی، دانشگاه آزاد اسلامی، واحد تهران مرکزی، تهران، ایرانموسیمظلومدانشکدهی مهندسی عمران، دانشگاه تربیت دبیر شهید رجایی، تهران، ایرانمجتبیجعفری صمیمیدانشکده مهندسی، دانشگاه آزاد اسلامی، واحد تهران مرکزی، تهران، ایرانمحمد حسنرامشتدانشکده مهندسی، دانشگاه آزاد اسلامی، واحد تهران مرکزی، تهران، ایرانJournal Article20220118<span style="letter-spacing: -.1pt;">Geopolymer concrete is an innovative building material that is produced by the chemical action of mineral molecules. Removal of cement is one of the great advantages of the use of geopolymer concrete. For this reason, to know the types of geopolymer concrete, it is important to examine its different components and their effect on fracture parameters. In this paper, the fracture parameters of lightweight geopolymer concrete based on class C fly ash (LWFCGC) are presented. In this research, three mix designs with the activator to binder ratios of 0.4, 0.5 and 0.6 were considered. By changing the ratio of activator to glue from 0.6 to 0.4, compressive strength from 18.9 MPa to 28.4 MPa, toughness from 14.07 MPa mm to 19.04 MPa mm 0.5, fracture energy from N/ 17.31 m to 20.98 N/m and the length of the fracture process area changed from 54.12 mm to 29.07 mm.</span>بتن متنوعترین و یکی از پرمصرفترین مصالح ساختمانی است. برای ساخت بتن به مقدار زیادی سیمان پرتلند نیاز است. تولید سیمان پرتلند همراه با تولید مقدار زیادی دی اکسید کربن است که جو را آلوده میکند. علاوه بر آن مقدار زیادی انرژی نیز برای تولید سیمان پرتلند مصرف میشود. از این رو، یافتن یک ماده جایگزین برای سیمان پرتلند اجتناب ناپذیر است. بتن ژئوپلیمری یک ماده ساختمانی نوآورانه است که از اثر شیمیایی مولکولهای معدنی تولید میشود. حذف سیمان پرتلند یکی از مزیتهای بزرگ استفاده از بتن ژئوپلیمری است. به همین دلیل برای شناخت انواع بتن ژئوپلیمری، مطالعه بر روی اجزای مختلف سازنده آن و تاثیر آنها بر پارامترهای شکست اهمیت دارد. در این مقاله نتایج آزمایشهای پارامترهای شکست بتن ژئوپلیمری سبک بر پایه خاکستر بادی کلاس C (Lightweight Fly ash C class-based Geopolymer Concrete) ارائه میشود. این آزمایشها شامل آزمایش خمش سه نقطهای بر روی 36 تیر با نسبت فعال کننده به چسب متفاوت است. همچنین آزمایشهای مقاومت فشاری و مقاومت کششی بر روی بتن سخت شده پس از گذشت 24 ساعت عملآوری انجام شد. در این آزمایشها سه طرح مخلوط با نسبت فعال کننده به چسب 0/4، 0/5 و 0/6 در نظر گرفته شد. با تغییر نسبت فعال کننده به چسب از 0/6 به 0/4، مقاومت فشاری از MPa 18/9 به MPa 28/4، چقرمگی از MPa mm<sup>0.5</sup> 19/04 به MPa mm<sup>0.5</sup>14/07، انرژی شکست از N/m 17/31 به N/m 20/98 و طول ناحیه فرایند شکست از mm 17/31 به mm 20/98 تغییر یافت.https://ceej.aut.ac.ir/article_5081_2d54dda4b19cfbae4242465a8431e531.pdf